性能項目 | 試驗條件[狀態] | 測試方法 | 測試數據 | 數據單位 | |
物理性能 | 比重 | ASTMD792 | 0.920 | g/cm3 | |
熔流率(熔體流動速率)(190°C/2.16kg) | ASTMD1238 | 0.90 | g/10min | ||
薄膜 | 薄膜厚度-經測試 | 25 | μm | ||
膜刺穿強度(25μm) | 內部方法 | 4.97 | J | ||
膜刺穿力(25μm) | 內部方法 | 53.4 | N | ||
膜耐刺穿性(25μm) | 內部方法 | 25.2 | J/cm3 | ||
膜強度 | MD:25μm | ASTMD882 | 113 | J/cm3 | |
TD:25μm | ASTMD882 | 131 | J/cm3 | ||
割線模量 | 1%正割,MD:25μm | ASTMD882 | 235 | MPa | |
2%正割,MD:25μm | ASTMD882 | 207 | MPa | ||
2%正割,MD:51μm | ASTMD882 | 173 | MPa | ||
1%正割,TD:25μm | ASTMD882 | 265 | MPa | ||
2%正割,TD:25μm | ASTMD882 | 225 | MPa | ||
2%正割,TD:51μm | ASTMD882 | 181 | MPa | ||
抗張強度 | MD:屈服,25μm | ASTMD882 | 10.8 | MPa | |
MD:屈服,51μm | ASTMD882 | 11.0 | MPa | ||
TD:屈服,25μm | ASTMD882 | 11.6 | MPa | ||
TD:屈服,51μm | ASTMD882 | 10.9 | MPa | ||
MD:斷裂,25μm | ASTMD882 | 45.4 | MPa | ||
MD:斷裂,51μm | ASTMD882 | 37.7 | MPa | ||
TD:斷裂,25μm | ASTMD882 | 41.6 | MPa | ||
TD:斷裂,51μm | ASTMD882 | 41.9 | MPa | ||
伸長率 | MD:斷裂,25μm | ASTMD882 | 570 | % | |
MD:斷裂,51μm | ASTMD882 | 580 | % | ||
TD:斷裂,25μm | ASTMD882 | 750 | % | ||
TD:斷裂,51μm | ASTMD882 | 720 | % | ||
落錘沖擊 | 25μm | ASTMD1709A | 210 | g | |
51μm | ASTMD1709A | 340 | g | ||
埃爾曼多夫抗撕強度 | MD:25μm | ASTMD1922 | 360 | g | |
MD:51μm | ASTMD1922 | 850 | g | ||
TD:25μm | ASTMD1922 | 640 | g | ||
TD:51μm | ASTMD1922 | 1100 | g | ||
薄膜厚度-經測試 | 25 | μm | |||
膜刺穿強度(25μm) | 內部方法 | 4.97 | J | ||
膜刺穿力(25μm) | 內部方法 | 53.4 | N | ||
膜耐刺穿性(25μm) | 內部方法 | 25.2 | J/cm3 | ||
膜強度 | MD:25μm | ASTMD882 | 113 | J/cm3 | |
TD:25μm | ASTMD882 | 131 | J/cm3 | ||
割線模量 | 1%正割,MD:25μm | ASTMD882 | 235 | MPa | |
2%正割,MD:25μm | ASTMD882 | 207 | MPa | ||
2%正割,MD:51μm | ASTMD882 | 173 | MPa | ||
1%正割,TD:25μm | ASTMD882 | 265 | MPa | ||
2%正割,TD:25μm | ASTMD882 | 225 | MPa | ||
2%正割,TD:51μm | ASTMD882 | 181 | MPa | ||
抗張強度 | MD:屈服,25μm | ASTMD882 | 10.8 | MPa | |
MD:屈服,51μm | ASTMD882 | 11.0 | MPa | ||
TD:屈服,25μm | ASTMD882 | 11.6 | MPa | ||
TD:屈服,51μm | ASTMD882 | 10.9 | MPa | ||
MD:斷裂,25μm | ASTMD882 | 45.4 | MPa | ||
MD:斷裂,51μm | ASTMD882 | 37.7 | MPa | ||
TD:斷裂,25μm | ASTMD882 | 41.6 | MPa | ||
TD:斷裂,51μm | ASTMD882 | 41.9 | MPa | ||
伸長率 | MD:斷裂,25μm | ASTMD882 | 570 | % | |
MD:斷裂,51μm | ASTMD882 | 580 | % | ||
TD:斷裂,25μm | ASTMD882 | 750 | % | ||
TD:斷裂,51μm | ASTMD882 | 720 | % | ||
落錘沖擊 | 25μm | ASTMD1709A | 210 | g | |
51μm | ASTMD1709A | 340 | g | ||
埃爾曼多夫抗撕強度 | MD:25μm | ASTMD1922 | 360 | g | |
MD:51μm | ASTMD1922 | 850 | g | ||
TD:25μm | ASTMD1922 | 640 | g | ||
TD:51μm | ASTMD1922 | 1100 | g | ||
熱性能 | 維卡軟化溫度 | ASTMD1525 | 107 | °C | |
溶融溫度(DSC) | 內部方法 | 119 | °C | ||
光學性能 | 光澤度 | 45°,25.4μm | ASTMD2457 | 41 | |
45°,50.8μm | ASTMD2457 | 81 | |||
霧度 | 25.4μm | ASTMD1003 | 16 | % | |
50.8μm | ASTMD1003 | 8.8 | % |